What Is Ferrosilicon Powdering?
Ferrosilicon powdering, also called disintegration, is the gradual crumbling of ferrosilicon lumps into powder during storage. It reduces product quality, increases dust losses and creates handling problems, so understanding its causes is important for producers and buyers.
Effect of Impurities
Improper amounts of aluminum, phosphorus and calcium in high carbon ferrosilicon all contribute to powdering. When the aluminum and phosphorus contents increase to a certain value at the same time, the ferrosilicon is prone to powdering in air with high humidity. Some data indicate that when the phosphorus content is below 0.04 percent and the aluminum content is below 3 percent, powdering is not easy to occur.
Effect of Silicon Content
Lower silicon content in ferrosilicon tends to cause powdering. The reason may be that the temperature of FeSi, FeSi2 and other silicon-iron compounds in ferrosilicon decreases and the volume expands, causing the alloy to disintegrate. Ferrosilicon containing aluminum forms aluminum hydroxide and generates gas when it meets water, which is the main reason for powdering of ferrosilicon.
Effect of Cooling Rate After Casting
The cooling rate after casting also affects powdering of ferrosilicon lumps. When the cooling speed of the alloy is fast, the segregation degree of silicon is small, so it is difficult to pulverize; when the cooling speed is slow, the segregation degree of silicon is large and pulverization easily occurs. By the same logic, thicker ferrosilicon ingots are prone to pulverization, while thinner ones are less likely to pulverize.
Prevention Measures
Control phosphorus below 0.04 percent and aluminum below 3 percent in high carbon grades; use faster cooling and thinner ingot cross sections to reduce silicon segregation; store in dry conditions and avoid long exposure to humid air; and keep packaging sealed and use desiccants where necessary.
Frequently Asked Questions
Why does ferrosilicon turn into powder? Mainly due to aluminum and phosphorus content reacting with moisture, low silicon content with phase volume changes, and slow cooling causing silicon segregation.
How can ferrosilicon powdering be prevented? By controlling impurities, faster cooling of ingots, dry storage and sealed packaging.
Which grades powder more easily? High carbon and lower silicon grades with higher aluminum and phosphorus content are more susceptible.
Why does aluminum promote powdering? aluminum-containing ferrosilicon forms aluminum hydroxide and generates gas when it meets water, which is the main reason for powdering of ferrosilicon.
How does the cooling rate affect powdering? Fast cooling reduces silicon segregation and makes pulverization difficult, while slow cooling increases silicon segregation and makes powdering more likely, which is why thicker ingots are more prone to disintegrate.