Jan 23, 2024 Leave a message

Ferrovanadium Production: Thermite and Silicothermic Routes

Thermite Method

Very early ferrovanadium production methods are still in use today, and aluminum is a strong reducing agent. The heat generated by reducing vanadium pentoxide with aluminum is quite large (4577 kJ per kg of mixture). Not only can the thermite smelting process be completed, but ferrovanadium waste can also be added back to the furnace to reduce the reaction temperature; lime, magnesia, and fluorite can be added to reduce the slag viscosity; the particle size of aluminum particles and vanadium pentoxide flakes can be adjusted to reduce the reaction speed, reduce splash loss, and increase the yield of vanadium.

The V2O5 content of the V2O5 fusible sheet is required to be at least 98 percent, with blockiness below 20 mm x 20 mm and plate thickness of 3-5 mm. Aluminum refers to aluminum particles with an aluminum content greater than 98 percent, a particle size less than 3 mm, and aluminum bubbles of 3-10 mm. The steel chips are ordinary carbon steel turning chips, with a roll length below 15 mm.

After the smelting reaction is completed, cool naturally for 16 to 24 hours. Pull out the furnace barrel, take out the iron vanadium ingot, clean, and package it. The composition of ferrovanadium obtained by smelting is: V 75-80 percent, Al 1-4 percent, Si 1.0-1.5 percent, C 0.13-0.2 percent, S at most 0.05 percent, P at most 0.075 percent. The slag mainly consists of V2O3, (CaO+MgO), and Al2O3. Ferrovanadium consumption to produce 1 t of 80 percent vanadium: 1500-1600 kg molten vanadium oxide (V2O5 98 percent) and 810-860 kg aluminum (Al 98 percent). The smelting recovery rate of vanadium is 90-95 percent.

In order to reduce the vanadium content in the slag, the slag is heated immediately after the reaction to cause the metal particles suspended in the slag to sink and continue to react with the vanadium oxide and residual aluminum in the slag to increase the recovery rate of vanadium.

Silicon Electrothermal Method

75 percent ferrosilicon and aluminum are used as reducing agents. Ferrovanadium with V 40-60 percent is produced in an improved three-phase alkaline electric arc furnace. The electric arc furnace transformer capacity is 1800 kVA, the operating voltage is 127/220 V, and the rated current is 4750 A. The graphite electrode diameter is 200 mm. Magnesia bricks are used as furnace linings, and the furnace cover is made of chrome magnesia bricks.

The raw materials used are: V2O5 fusion plate (V2O5 at least 98 percent, Si at most 0.25 percent, iron at most 0.30 percent, P at most 0.05 percent, S at most 0.03 percent, As at most 0.02 percent, Na2O+K2O at most 1.5 percent, plate thickness about 8.0 mm, fragment size at most 200 mm x 200 mm); ferrosilicon (75 percent ferrosilicon, block at most 30 mm); aluminum block (process aluminum ingot to at most 20 mm); lime (CaO at least 85 percent, P at most 0.015 percent, block size 30-50 mm); and scrap steel or steel scraps of ordinary carbon steel.

Frequently Asked Questions

What is the thermite method? Reduction of vanadium pentoxide by aluminum, using the reaction heat for smelting.

What vanadium recovery is achieved? 90-95 percent by the thermite route.

What is the silicon electrothermal method? Reduction with 75 percent ferrosilicon and aluminum in a three-phase electric arc furnace, producing FeV 40-60 percent.