Tungsten trioxide may be slightly reduced to blue tungsten oxide in hydrogen at about 450°C. To make tungsten filament for incandescent lamp filaments, a small amount of potassium oxide, silicon oxide and aluminum oxide must be mixed with tungsten trioxide or blue tungsten oxide. The total amount of the three does not exceed 1%. This is the tungsten invented by Baz in 1922. Silk doping process.

fine tungsten wire
The doped tungsten oxide is reduced to metallic tungsten powder with hydrogen gas. The reduction process is generally carried out in two steps: the first step is reduced to tungsten dioxide (brown tungsten oxide) at around 630°C, and the second step is reduced to metallic tungsten powder at around 820°C. The purpose of the two-step reduction is to allow the incorporated potassium to fully exert its effect and to control the powder particle size. The doped tungsten powder obtained in this way is then pressed into elongated square bars in a special mold.

fine w wire