(1) It is necessary to control the heating rate of different firing temperature ranges. The heating rate slows down when it is less than 600℃. The heating rate can be accelerated when it is between 600 and 1000℃. The heating rate should be slow when between 1100 and 1300℃. When it is between 1300℃ and the firing temperature (1430℃ to 1450℃), the heating rate should be the highest during the firing process. The slowest among them. The fired silica bricks should be cooled below 600°C, especially slowly at 300°C. This can effectively buffer the volume change of crystalline transformation, make the tridymite and cristobalite content higher, and avoid the formation of cracks.

(2) A reducing atmosphere should be used in the high-temperature firing stage to facilitate the mineralization of low-priced iron oxide and promote the large-scale formation of tridymite. Otherwise, in an oxidizing atmosphere, especially when the mineralizer is insufficient, α-quartz is mostly converted into α-cristobalite. This transformation is called "dry transformation".

During dry conversion, due to the uneven volume expansion of the bricks and the lack of liquid buffer stress, the structure of the product will be loose and cracked. At the same time, appropriate insulation should be carried out at different temperature stages of silica brick firing so that the silica bricks have a reasonable phase composition and meet the use requirements.

(3) Improve the semi-finished product loading system to reduce the probability of cracks. Transverse cracks in silica bricks, that is, cracks parallel to the pressure direction of the product, are usually caused by uneven heating of various parts when the product is fired. They often appear on the fire surface outside the brick stack, especially on the top surface of the product. As for the reticular cracks on the surface of silica bricks, in addition to the microscopic unevenness of the green body itself due to uneven kneading or changes in raw materials, it is usually caused by the product being heated to an excessively high temperature and with large fluctuations.

When loading, the special-shaped silica bricks need to be placed inside the kiln car, and the standard ordinary bricks should be installed on the outside of the kiln car; the protruding parts of the special-shaped bricks or the parts prone to cracks should be inward; the top of the kiln car should be covered with some Thin bricks to avoid direct impact of flames, otherwise it will lead to increased cracks.